Materials · Steel
Steel — EN 10025 (Europe)
Specified minimum or characteristic values, for preliminary design. They vary with thickness, class and edition of the standard: check the reference text.
| Material | FyMPa | FuMPa | EMPa | GMPa | ν | ρkg/m³ | α10⁻⁶/°C | Reference |
|---|---|---|---|---|---|---|---|---|
| S235 | 235 | 360 | 200,000 | 77,000 | 0.3 | 7,850 | 11.7 | EN 10025-2 · EN 1993-1-1 Table 3.1, t ≤ 40 mm |
| S275 | 275 | 430 | 200,000 | 77,000 | 0.3 | 7,850 | 11.7 | EN 10025-2 · EN 1993-1-1 Table 3.1, t ≤ 40 mm |
| S355 | 355 | 490 | 200,000 | 77,000 | 0.3 | 7,850 | 11.7 | EN 10025-2 · EN 1993-1-1 Table 3.1, t ≤ 40 mm |
| S450 | 440 | 550 | 200,000 | 77,000 | 0.3 | 7,850 | 11.7 | EN 10025-2 · EN 1993-1-1 Table 3.1, t ≤ 40 mm |
| S275 N/NL | 275 | 390 | 200,000 | 77,000 | 0.3 | 7,850 | 11.7 | EN 10025-3 · EN 1993-1-1 Table 3.1, t ≤ 40 mm |
| S355 N/NL | 355 | 490 | 200,000 | 77,000 | 0.3 | 7,850 | 11.7 | EN 10025-3 · EN 1993-1-1 Table 3.1, t ≤ 40 mm |
| S420 N/NL | 420 | 520 | 200,000 | 77,000 | 0.3 | 7,850 | 11.7 | EN 10025-3 · EN 1993-1-1 Table 3.1, t ≤ 40 mm |
| S460 N/NL | 460 | 540 | 200,000 | 77,000 | 0.3 | 7,850 | 11.7 | EN 10025-3 · EN 1993-1-1 Table 3.1, t ≤ 40 mm |
| S460 M/ML | 460 | 540 | 200,000 | 77,000 | 0.3 | 7,850 | 11.7 | EN 10025-4 · EN 1993-1-1 Table 3.1, t ≤ 40 mm |